InAsSb - Indium Arsenide Antimonide

Basic Parameters at 300 K

Crystal structure Zinc Blende
Group of symmetry Td2-F43m
Number of atoms in 1 cm3 (3.59-0.65x)·1022
Density 5.68+0.09x g·cm-3
Dielectric constant (static) 15.15+1.65x
Dielectric constant (high frequency) 12.3+3.4x
Effective electron mass me 0.023-0.039x+0.03x2 mo
Effective hole masses mh 0.41+0.02x mo
Effective hole masses mlp 0.026-0.011 mo
Electron affinity 4.9-0.31x eV
Lattice constant 6.0583+0.4207 A