| Index of refraction | 2.4 |
| Radiative recombination coefficient | 9·105cm3/s |
Infrared refractive index n=2.375.
![]() |
Type IIa diamond refractive index versus wavelength. Experimental points: data from four references (Edwards and Ochoa [1981]). |
![]() |
Type IIa diamond refractive index versus photon energy at 300 K. (Walker and Osantowski [1964]). |
![]() |
Reflectance versus photon energy, 300 K. (Walker and Osantowski [1964]). |
![]() |
Absorption edge spectrum of diamond at various temperatures. (Clark et al. [1964]). |
![]() |
Visible and ultraviolet absorption spectra of a diamond with different types of impurities. Predominant type of impurity is: 1. boron atoms; 2. N3 centers; 3. single nitrogen atoms; 4. absorption spectra of a brown diamond. (Wilks and Wilks [1991]). |
![]() |
Infrared absorption spectra of a diamond in which 1. boron atoms are predominant impurities; 2. single nitrogen atoms are predominant impurities (Wilks and Wilks [1991]). |
| λ | τp, ns | β×1011, m W-1 |
| 0.248 | 0.0005 | 1.6±0.3 |
| 0.31 | 0.000135 | 0.75±0.15 |
| 0.3547 | 0.015 | 0.3 |
| 0.5321 | 0.03 | <0.26 |