| Bulk modulus | 5.8·1011 dyn cm-2 |
| Melting point | 942 °C |
| Specific heat | 0.25 J g-1 °C-1 |
| Thermal conductivity | 0.27 W cm-1 °C-1 |
| Thermal diffusivity | 0.19 cm2s-1 |
| Thermal expansion, linear | 4.52·10-6 °C-1 |
![]() |
Temperature dependence of thermal conductivity. n-type sample, no (cm-3): 1. 1.6·1016; 2. 2.0·1017; p-type sample, po (cm-3): 3. 2.0·1017. (Tamarin and Shalyt [1971]). |
![]() |
Temperature dependences of thermal conductivity for high temperatures Electron concentration no (cm-3): 1. 5·1016; 2. 2·1016; 3. 3·1016. (Okhotin et al. [1972]). |
![]() |
Temperature dependence of specific heat at constant pressure (Piesbergen[1963]). |
Cp= 0.240 + 3.97·10-5·T (J g-1°C -1).(Barin et al. [1977]).
![]() |
Temperature dependence of linear expansion coefficient (low temperature) (Sparks and Swenson[1967]). |
![]() |
Temperature dependence of linear expansion coefficient
(high temperature) (Sirota and Berger[1959]). |
![]() |
Temperature dependences of Nernst coefficient (transverse Nernst-Ettinghausen effect) Electron concentration at 77K no (cm-3): 1. 2.96·1016; 2. 4.46·1016; 3. 8.43·1016; 4. 4.53·1017; 5. 1.56·1018; 6. 2.28·1018; 7. 5·1018; 8. 1.68·1019. (Domanskaya et al. [1970]). |
for 950 K - 2·10-3,
for 1000 K - 10-2,
for 1050 K - 10-1.