| Crystal structure | Diamond |
| Group of symmetry | Oh7-Fd3m |
| Number of atoms in 1 cm3 | 5·1022 |
| Auger recombination coefficient Cn | 1.1·10-30 cm6 s-1 |
| Auger recombination coefficient Cp | 3·10-31cm6 s-1 |
| Debye temperature | 640 K |
| Density | 2.329 g cm-3 |
| Dielectric constant | 11.7 |
| Effective electron masses ml | 0.98mo |
| Effective electron masses mt | 0.19mo |
| Effective hole masses mh | 0.49mo |
| Effective hole masses mlp | 0.16mo |
| Electron affinity | 4.05 eV |
| Lattice constant | 5.431 A |
| Optical phonon energy | 0.063 eV |